B1246 of 55
0 XP
  1. Hook
  2. Play
  3. Predict
  4. Name it
  5. Check
  6. Explain

B12 · Lesson 46 · Crystal growth

How silicon boules are pulled from the melt, why dopants and impurities spread unevenly along them, and how zone refining purifies

Nearly every silicon wafer starts as a single crystal pulled slowly out of a crucible of molten silicon, a boule two meters long and 300 mm across. Dopant added to the melt doesn't freeze into the crystal at the melt's concentration: most dopants prefer to stay in the liquid, so the melt gets richer as the boule grows, and the crystal's far end is doped more heavily than its seed end. The same preference is what lets zone refining sweep impurities out of a crystal, and it's the binary phase diagram of B11.35 seen at its dilute corner.

  • The curve is the dopant concentration frozen into a boule, relative to the starting melt's, against the fraction of the melt that has solidified (Scheil's law), on a log scale.
  • The slider sets the segregation coefficient k: about 0.8 for boron, 0.35 for phosphorus, 0.3 for arsenic and 0.023 for antimony.
  • The readouts compare the two ends. A k near 1 makes the boule uniform; a small k makes its last part far richer than its first.

Predict

A silicon boule is grown from a melt doped with phosphorus (k = 0.35). How does the phosphorus in the crystal change from the seed end to the far end?

Name it

Segregation

At a growing crystal's interface, the solid and liquid don't take the same concentration of a dilute impurity: the equilibrium segregation coefficient is k0=CsCl. In silicon it's 0.8 for boron, 0.35 for phosphorus, 0.3 for arsenic, 0.023 for antimony, and 10−5 or less for metals like iron and gold. Below 1 means the impurity lowers the melting point, and the crystal rejects it into the melt.

Normal freezing

If the melt stays well mixed and the solid doesn't diffuse, a mass balance gives Scheil's law for the concentration frozen in when a fraction f has solidified:

Cs=kC0(1−f)k−1,

with C0 the starting melt concentration. The melt itself enriches as Cl=C0(1−f)k−1.

Effective segregation

A growing crystal rejects impurity faster than diffusion carries it away, so a layer enriched in impurity builds up ahead of the interface. Burton, Prim and Slichter found

keff=k0k0+(1−k0)e−vδ/D,

with growth rate v, boundary-layer thickness δ and diffusion constant D in the melt. Fast growth or poor stirring pushes keff toward 1. Rotating the crystal and crucible controls δ, and with it the doping.

Zone refining

Passing a narrow molten zone of length L along a solid bar sweeps impurities with k < 1 toward the end. After one pass the concentration a distance x from the start is

C=C0[1−(1−k)e−kx/L].

Many passes purify further. Float-zone silicon, grown with no crucible at all, is made this way and reaches resistivities over 10 kΩ·cm; Czochralski silicon picks up about 1018 oxygen atoms per cm³ from its quartz crucible, which later precipitates and helps getter metal impurities.

Worked example

Compare the doping along phosphorus-doped (k = 0.35) and boron-doped (k = 0.8) Czochralski boules at the seed end, halfway and 90% solidified.

Show the solution
  1. Segregation formula. Cs=kC0(1−f)k−1
  2. Phosphorus. At the seed end, halfway and 90% solidified, the doping is 0.350, 0.549 and 1.563 times C0.
  3. Boron. At the same points it's 0.800, 0.919 and 1.268 times C0.
  4. Compare. The phosphorus boule's doping rises 4.5 times from the seed to 90%; the boron boule's 1.6 times.
  5. What it means for resistivity. Resistivity goes inversely, so a phosphorus boule specified at 10 Ω·cm must be cut into narrow ranges, or grown with the melt replenished continuously to hold its concentration steady.

Answer phosphorus runs 0.350, 0.549 and 1.563 times C0 and boron 0.800, 0.919 and 1.268 times C0, so the phosphorus doping varies far more along the boule.

Worked example

A silicon bar contains iron (k = 8 × 10⁻⁶) and boron (k = 0.8). After one zone-refining pass, how much of each remains one zone length from the start?

Show the solution
  1. One zone length in. At x = L, C/C0=1−(1−k)e−k
  2. Iron. CC0=1−(1−8×10−6)e−8×10−6=1.6×10−5 One pass removes it 60 000-fold.
  3. Boron. CC0=1−0.2e−0.8=0.91 barely any change.
  4. The pattern. Impurities with k far from 1 are easy to sweep out; those with k near 1, like boron, hardly move.
  5. What it means for silicon. That's why boron has to be removed chemically before silicon is grown, and why the purest silicon is float-zone material, refined with no crucible to add contamination.

Answer after one pass, 1.6×10−5 of the iron remains and 0.91 of the boron.

Worked example

Phosphorus (k₀ = 0.35, D = 10⁻⁴ cm²/s in the melt) is grown into a crystal at 1 mm/min with a 0.5 mm boundary layer. What's its effective segregation coefficient?

Show the solution
  1. Growth speed. 1 mm/min is 1.67×10−5 m/s.
  2. Boundary-layer parameter. vδD=1.67×10−5×5×10−410−8=0.833
  3. Effective coefficient. keff=0.350.35+0.65e−0.833=0.55
  4. Growth conditions. Growing faster or stirring less would push it further toward 1.
  5. Striations. Variations in growth rate, from temperature fluctuations, leave rings of varying doping across the wafer, called striations, which show up in resistivity maps.

Answer the effective segregation coefficient is 0.55.

Check

A boule is grown from a well-mixed melt with segregation coefficient 0.35, and a fraction 0.2 has solidified.

(a)

What's the concentration being frozen in, relative to the starting melt?

(b)

How many times the seed end's concentration is that?

Check

After one zone-refining pass, what fraction of an impurity with k = 0.023 remains 0.5 zone lengths from the start?

Check

A crystal grows at 0.5 mm/min with a 1 mm boundary layer, for an impurity with k0 = 0.023 and D = 10⁻⁴ cm²/s in the melt. What's its effective segregation coefficient?

Check

A boule doped with k = 0.35 has resistivity 20 Ω·cm at its seed end.

(a)

What's its resistivity where a fraction 0.5 has solidified (mobility unchanged)?

Write units the way you normally would: 1.5 Ω·cm, 1500 mΩ·cm and 0.0015 kΩ·cm are the same answer.

(b)

At what solidified fraction does the crystal's doping equal the starting melt's?

Check

A silicon crystal's interface releases latent heat (1.8 MJ/kg, density 2330 kg/m³) that must be conducted away. If 10 W/cm² can be removed, how fast can it grow?

Write units the way you normally would: 1.5 mm/min, 1500 µm/min and 0.0015 m/min are the same answer.

Check

Why are boron-doped silicon boules more uniform along their length than antimony-doped ones?

Check

A melt with segregation coefficient k has solidified a fraction f under normal freezing.

Step 1

What's the liquid's concentration, relative to its start?

Type it the way you would write it, like 3sin(2πft) or 3*sin(2*pi*f*t). Angles can be in radians or carry a degree sign, like 45°.

Check

Write freeze(k, n) simulating normal freezing in n equal steps: at each step, freeze 1/n of the original melt at k times the current liquid concentration (starting at 1) and update the liquid by mass balance; the last step freezes everything left, impurity and all. Return a list of the solid concentrations.

Python 3.14 with numpy and matplotlib, running in your browser. Tab indents; press Esc and then Tab to move on.

Explain why

Why does an impurity that lowers a material's melting point tend to stay in the liquid when it freezes?

Practice

Keep practicing

7 kinds of problem on this topic, dealt one at a time with new numbers every time, for as long as you like.