title: Crystal growth and segregation
heading: How silicon boules are pulled from the melt, why dopants and impurities spread unevenly along them, and how zone refining purifies
eyebrow: B12 · Lesson 46 · Crystal growth
xp: 40
---

::: hook
Nearly every silicon wafer starts as a single crystal pulled slowly out of a crucible of molten silicon, a boule two meters long and 300 mm across. Dopant added to the melt doesn't freeze into the crystal at the melt's concentration: most dopants prefer to stay in the liquid, so the melt gets richer as the boule grows, and the crystal's far end is doped more heavily than its seed end. The same preference is what lets zone refining sweep impurities out of a crystal, and it's the binary phase diagram of B11.35 seen at its dilute corner.
:::

::: play
- The curve is the dopant concentration frozen into a boule, relative to the starting melt's, against the fraction of the melt that has solidified (Scheil's law), on a log scale.
- The slider sets the segregation coefficient k: about 0.8 for boron, 0.35 for phosphorus, 0.3 for arsenic and 0.023 for antimony.
- The readouts compare the two ends. A k near 1 makes the boule uniform; a small k makes its last part far richer than its first.
:::

```sim plot
view: graph
x: f = 0..0.95
y: C = 0.1..10 log
slider: k = 0.01..1 step 0.005 = 0.35
plot: k*(1 - f)^(k - 1) | label: dopant in the crystal ÷ starting melt | samples: 300
marker: C = 1 | label: starting melt
readout: seed end, C/C₀ = k | digits: 3
readout: at 90% solidified, C/C₀ = k*0.1^(k - 1) | digits: 3
readout: ratio, 90% to seed = 0.1^(k - 1) | digits: 3
```

::: predict
## A silicon boule is grown from a melt doped with phosphorus (k = 0.35). How does the phosphorus in the crystal change from the seed end to the far end?

- [ ] It's uniform along the boule
- [ ] It falls toward the far end
- [x] It rises steadily, to several times the seed end's
- [ ] It rises at first, then falls

::: reveal
It rises steadily. The crystal takes only 35% of the melt's concentration at the interface, so phosphorus piles up in the shrinking melt. By the time 90% has frozen the crystal is 4.5 times as heavily doped as at the seed, and its resistivity is 4.5 times lower. Boron, with k = 0.8, varies only 1.6 times, which is one reason p-type wafers come out more uniform.
:::
:::

::: nameit
## Segregation

At a growing crystal's interface, the solid and liquid don't take the same concentration of a dilute impurity: the equilibrium segregation coefficient is $k_0 = \frac{C_s}{C_l}$. In silicon it's 0.8 for boron, 0.35 for phosphorus, 0.3 for arsenic, 0.023 for antimony, and $10^{-5}$ or less for metals like iron and gold. Below 1 means the impurity lowers the melting point, and the crystal rejects it into the melt.

## Normal freezing

If the melt stays well mixed and the solid doesn't diffuse, a mass balance gives Scheil's law for the concentration frozen in when a fraction f has solidified:

$$C_s = kC_0(1 - f)^{k - 1},$$

with $C_0$ the starting melt concentration. The melt itself enriches as $C_l = C_0(1 - f)^{k - 1}$.

## Effective segregation

A growing crystal rejects impurity faster than diffusion carries it away, so a layer enriched in impurity builds up ahead of the interface. Burton, Prim and Slichter found

$$k_{eff} = \frac{k_0}{k_0 + (1 - k_0)e^{-v\delta/D}},$$

with growth rate v, boundary-layer thickness δ and diffusion constant D in the melt. Fast growth or poor stirring pushes $k_{eff}$ toward 1. Rotating the crystal and crucible controls δ, and with it the doping.

## Zone refining

Passing a narrow molten zone of length L along a solid bar sweeps impurities with k < 1 toward the end. After one pass the concentration a distance x from the start is

$$C = C_0\left[1 - (1 - k)e^{-kx/L}\right].$$

Many passes purify further. Float-zone silicon, grown with no crucible at all, is made this way and reaches resistivities over 10 kΩ·cm; Czochralski silicon picks up about $10^{18}$ oxygen atoms per cm³ from its quartz crucible, which later precipitates and helps getter metal impurities.
:::

::: example
## Compare the doping along phosphorus-doped (k = 0.35) and boron-doped (k = 0.8) Czochralski boules at the seed end, halfway and 90% solidified.

::: solution
1. **Segregation formula.**
   $$C_s = kC_0(1 - f)^{k - 1}$$
2. **Phosphorus.** At the seed end, halfway and 90% solidified, the doping is 0.350, 0.549 and 1.563 times $C_0$.
3. **Boron.** At the same points it's 0.800, 0.919 and 1.268 times $C_0$.
4. **Compare.** The phosphorus boule's doping rises 4.5 times from the seed to 90%; the boron boule's 1.6 times.
5. **What it means for resistivity.** Resistivity goes inversely, so a phosphorus boule specified at 10 Ω·cm must be cut into narrow ranges, or grown with the melt replenished continuously to hold its concentration steady.

**Answer:** phosphorus runs 0.350, 0.549 and 1.563 times $C_0$ and boron 0.800, 0.919 and 1.268 times $C_0$, so the phosphorus doping varies far more along the boule.
:::
:::

::: example
## A silicon bar contains iron (k = 8 × 10⁻⁶) and boron (k = 0.8). After one zone-refining pass, how much of each remains one zone length from the start?

::: solution
1. **One zone length in.** At x = L,
   $$C/C_0 = 1 - (1 - k)e^{-k}$$
2. **Iron.**
   $$\begin{aligned} \frac{C}{C_0} &= 1 - (1 - 8 \times 10^{-6})e^{-8 \times 10^{-6}} \\ &= 1.6 \times 10^{-5} \end{aligned}$$
   One pass removes it 60 000-fold.
3. **Boron.**
   $$\begin{aligned} \frac{C}{C_0} &= 1 - 0.2e^{-0.8} \\ &= 0.91 \end{aligned}$$
   barely any change.
4. **The pattern.** Impurities with k far from 1 are easy to sweep out; those with k near 1, like boron, hardly move.
5. **What it means for silicon.** That's why boron has to be removed chemically before silicon is grown, and why the purest silicon is float-zone material, refined with no crucible to add contamination.

**Answer:** after one pass, $1.6 \times 10^{-5}$ of the iron remains and 0.91 of the boron.
:::
:::

::: example
## Phosphorus (k₀ = 0.35, D = 10⁻⁴ cm²/s in the melt) is grown into a crystal at 1 mm/min with a 0.5 mm boundary layer. What's its effective segregation coefficient?

::: solution
1. **Growth speed.** 1 mm/min is $1.67 \times 10^{-5}$ m/s.
2. **Boundary-layer parameter.**
   $$\begin{aligned} \frac{v\delta}{D} &= \frac{1.67 \times 10^{-5} \times 5 \times 10^{-4}}{10^{-8}} \\ &= 0.833 \end{aligned}$$
3. **Effective coefficient.**
   $$\begin{aligned} k_{eff} &= \frac{0.35}{0.35 + 0.65e^{-0.833}} \\ &= 0.55 \end{aligned}$$
4. **Growth conditions.** Growing faster or stirring less would push it further toward 1.
5. **Striations.** Variations in growth rate, from temperature fluctuations, leave rings of varying doping across the wafer, called striations, which show up in resistivity maps.

**Answer:** the effective segregation coefficient is 0.55.
:::
:::

::: check
kind: parts
given: k = 0.023 | 0.35 | 0.8; f = 0.2 | 0.5 | 0.8

## A boule is grown from a well-mixed melt with segregation coefficient {k}, and a fraction {f} has solidified.

::: part
answer: k*(1 - f)^(k - 1)
tolerance: 0.5%

### What's the concentration being frozen in, relative to the starting melt?

::: misses
- [k] That's only at the seed end; the melt has since enriched.
- [any] $C_s = kC_0(1 - f)^{k - 1}$.
:::
:::

::: part
answer: (1 - f)^(k - 1)
tolerance: 0.5%

### How many times the seed end's concentration is that?

::: misses
- [any] Divide by $kC_0$.
:::
:::
:::

::: check
given: k = 0.00001 | 0.023 | 0.35 | 0.8; x = 0.5 | 1 | 3
answer: 1 - (1 - k)*exp(-k*x)
tolerance: 0.5%

## After one zone-refining pass, what fraction of an impurity with k = {k} remains {x} zone lengths from the start?

::: right
Right. $1 - (1 - k)e^{-kx/L}$.
:::

::: misses
- [k] That's just at the very start; farther along, the zone has picked up impurity.
- [any] $C/C_0 = 1 - (1 - k)e^{-kx/L}$.
:::
:::

::: check
given: k = 0.023 | 0.35; v = 0.5 | 2; d = 0.1 | 1
answer: k/(k + (1 - k)*exp(-v/60*d*1e-1/1e-4))
tolerance: 0.5%

## A crystal grows at {v} mm/min with a {d} mm boundary layer, for an impurity with $k_0$ = {k} and D = 10⁻⁴ cm²/s in the melt. What's its effective segregation coefficient?

::: right
Right. $k_{eff} = \frac{k_0}{k_0 + (1 - k_0)e^{-v\delta/D}}$.
:::

::: misses
- [k] At this growth rate the interface layer matters.
- [any] Burton–Prim–Slichter, with $\frac{v\delta}{D}$ in consistent units.
:::
:::

::: check
kind: parts
given: k = 0.3 | 0.35 | 0.8; f = 0.5 | 0.9; r = 5 | 20

## A boule doped with k = {k} has resistivity {r} Ω·cm at its seed end.

::: part
answer: r*(1 - f)^(1 - k)
unit: Ω·cm
tolerance: 0.5%

### What's its resistivity where a fraction {f} has solidified (mobility unchanged)?

::: misses
- [r*(1 - f)^(k - 1)] Resistivity falls as the doping rises.
- [any] ρ ∝ 1/C, and C rises as $(1 - f)^{k - 1}$.
:::
:::

::: part
answer: 1 - k^(1/(1 - k))
tolerance: 0.5%

### At what solidified fraction does the crystal's doping equal the starting melt's?

::: misses
- [any] Solve $k(1 - f)^{k - 1} = 1$.
:::
:::
:::

::: check
given: q = 5 | 10 | 20
answer: q*1e4/(2330*1.8e6)*1000*60
unit: mm/min
tolerance: 0.5%

## A silicon crystal's interface releases latent heat (1.8 MJ/kg, density 2330 kg/m³) that must be conducted away. If {q} W/cm² can be removed, how fast can it grow?

::: right
Right. $v = \frac{q}{\rho L}$: growth is limited by removing latent heat.
:::

::: misses
- [q/(2330*1.8e6)*1000*60] Convert W/cm² to W/m².
- [any] $v = \frac{q}{\rho L}$.
:::
:::

::: check
kind: choice

## Why are boron-doped silicon boules more uniform along their length than antimony-doped ones?

- [ ] Boron diffuses faster in the solid
- [x] Boron's segregation coefficient is near 1, so the melt barely enriches as the crystal grows
- [ ] Antimony evaporates from the melt
- [ ] Boron atoms are smaller

::: right
Right. With k = 0.8 the crystal takes almost the melt's concentration; with k = 0.023 nearly all the antimony stays behind and the melt's concentration climbs.
:::

::: misses
- [1] Solid-state diffusion is far too slow to even out a boule.
- [3] Antimony does evaporate somewhat, but segregation dominates the profile.
- [4] Atomic size affects k, but the uniformity follows from k itself.
:::
:::

::: check
kind: derivation
vars: k = 0.01..0.99, f = 0.01..0.99

## A melt with segregation coefficient k has solidified a fraction f under normal freezing.

::: step
answer: (1 - f)^(k - 1)

### What's the liquid's concentration, relative to its start?
:::

::: step
answer: k*(1 - f)^(k - 1)

### What's the solid being frozen now?
:::

::: step
answer: (1 - (1 - f)^k)/f

### What's the average concentration of all the solid so far?
:::

::: right
Right. The average times f plus the liquid's share times (1 − f) adds back to 1: no impurity is lost.
:::
:::

::: check
kind: python

## Write `freeze(k, n)` simulating normal freezing in n equal steps: at each step, freeze 1/n of the original melt at k times the current liquid concentration (starting at 1) and update the liquid by mass balance; the last step freezes everything left, impurity and all. Return a list of the solid concentrations.

```python starter
def freeze(k, n):
    return [k] * n

print(freeze(0.35, 1000)[499])
```

```python solution
def freeze(k, n):
    liquid = 1.0
    mass = 1.0
    out = []
    dm = 1.0 / n
    for i in range(n - 1):
        cs = k * liquid
        out.append(cs)
        total = liquid * mass - cs * dm
        mass -= dm
        liquid = total / mass
    out.append(liquid)
    return out

print(freeze(0.35, 1000)[499])
```

```python tests
cs = freeze(0.35, 10000)
assert abs(cs[0] - 0.35) < 1e-12, "The first solid is k times the starting melt."
assert abs(cs[4999] / (0.35 * 0.5**(0.35 - 1)) - 1) < 2e-3, f"Halfway, Scheil gives 0.549; got {cs[4999]}"
assert abs(cs[8999] / (0.35 * 0.1**(0.35 - 1)) - 1) < 5e-3, "At 90% it gives 1.563."
assert abs(sum(cs) / len(cs) - 1) < 0.02, "Averaged over the whole boule, the doping matches the melt."
```

::: right
Right. Small steps reproduce Scheil's law, and the totals check that nothing is lost.
:::
:::

::: explain
## Why does an impurity that lowers a material's melting point tend to stay in the liquid when it freezes?

::: model
An impurity lowers the melting point when it's more comfortable dissolved in the liquid than in the solid: the liquid accommodates it with less strain or a better bonding arrangement, so its chemical potential is lower there. In equilibrium the impurity's chemical potential must be the same in both phases, which requires a lower concentration in the solid than in the liquid, a segregation coefficient below 1. As the crystal grows, it keeps rejecting the impurity into the melt, which gets steadily richer. The same equilibrium, seen on the phase diagram, is a liquidus line sloping down from the pure material's melting point.
:::
:::

::: practice

::: check
given: k = 0.3 | 0.8; f = 0.3 | 0.7
answer: k*(1 - f)^(k - 1)
tolerance: 0.5%

## Scheil concentration for k = {k} at f = {f}?

::: misses
- [any] $kC_0(1 - f)^{k - 1}$.
:::
:::

::: check
given: k = 0.001 | 0.5; x = 1 | 2
answer: 1 - (1 - k)*exp(-k*x)
tolerance: 0.5%

## One zone pass, k = {k}, at x = {x}L?

::: misses
- [any] $1 - (1 - k)e^{-kx/L}$.
:::
:::
:::