B12 · Lesson 37 · Magnetism in solids
Ferromagnets, hysteresis, and the materials in every inductor and motor
B11 explained paramagnetism: independent spins weakly lining up with a field. In iron, cobalt, nickel and the ferrites, the exchange interaction, a quantum effect of the Pauli principle on neighboring electrons, aligns spins spontaneously, without any field, below a Curie temperature. That spontaneous order is what makes transformer cores, inductors, motors and permanent magnets possible. Real magnets break into domains, and the way domain walls move and stick produces hysteresis: the loop whose shape separates soft materials, which should switch easily and waste little energy per cycle, from hard ones, which should hold their magnetization against anything.
- A model hysteresis loop: magnetization against applied field, with saturation , coercive field (where the magnetization crosses zero) and a softness w.
- The area enclosed is the energy lost as heat per cycle per unit volume: exactly for this shape. A transformer core cycles it fifty or a hundred thousand times a second.
- Shrink toward zero: a soft magnet, ideal for cores. Raise it: a hard magnet, ideal for motors and speakers.
Predict
Iron has about 8.5 × 10²⁸ atoms per m³, each contributing about 2.2 Bohr magnetons. What's its saturation flux density, ?
= 1.75 × 10⁶ A/m, and = 2.2 T. That's why iron-based cores saturate near 2 T, and why a power transformer can't be shrunk by simply running it at higher flux: past saturation the core stops helping and the magnetizing current soars.
Name it
Kinds of magnetism
- Diamagnetism: every material weakly opposes an applied field (induced orbital currents).
- Paramagnetism: independent moments align weakly with a field, χ ∝ 1/T (B11.7).
- Ferromagnetism: exchange aligns neighboring spins spontaneously below the Curie temperature: Fe 1043 K, Co 1388 K, Ni 627 K, NdFeB about 590 K, ferrites 400 to 700 K.
- Antiferromagnetism and ferrimagnetism: neighbors align oppositely; in ferrites the two sublattices are unequal, leaving a net moment. Ferrites are insulators, so eddy currents vanish, which is why they're used at high frequency.
Saturation
With n magnetic atoms per volume each carrying p Bohr magnetons ( = 9.274 × 10⁻²⁴ J/T), . Saturation flux densities: iron 2.15 T, silicon steel about 2.0, nickel–iron alloys 0.8 to 1.6, ferrites 0.3 to 0.5.
Domains and hysteresis
A large crystal splits into domains to reduce its stray-field energy. Magnetizing it moves domain walls and rotates domains; defects pin the walls, so the magnetization lags the field, tracing a loop. Key numbers: remanence (flux at zero field), coercivity (field to bring it to zero), and the loop area, the energy dissipated per cycle per volume: about for a square loop.
Soft and hard
- Soft ( from 0.5 to 100 A/m): silicon steel, nickel–iron, amorphous metals, ferrites, for transformers, inductors and shields.
- Hard ( around 10⁶ A/m): NdFeB ( ≈ 1.3 T), SmCo, hard ferrite, for motors and speakers. The figure of merit is the maximum energy product , at most : 336 kJ/m³ for = 1.3 T.
Spintronics
Electrons' spin also affects resistance: giant and tunneling magnetoresistance, where a stack's resistance depends on whether two magnetic layers are parallel, read every hard-disk bit and store data in MRAM.
Worked example
A ferrite core with = 0.5 T and = 10 A/m is driven through its full loop at 100 kHz. How much power does each cm³ lose to hysteresis?
Show the solution
- Loss per cycle.
- Loss per second. At 10⁵ cycles per second,
- In a real converter. A real converter drives the core through a small loop, perhaps ±0.1 T, and loses roughly ten times less, but loss still grows with frequency, which is why switching frequencies and core materials are chosen together.
Answer each cm³ loses 2 W to hysteresis.
Worked example
A 230 V, 50 Hz transformer winding has 500 turns on a 20 cm² core. What peak flux density does it reach?
Show the solution
- Transformer equation. For a sinusoid, , so
- Compare with saturation. That's comfortably below silicon steel's 2 T saturation, leaving margin for overvoltage.
Answer the peak flux density is 1.04 T.
Worked example
A hard-disk bit's magnetic grains must stay put for ten years, which needs . With anisotropy K = 0.5 MJ/m³ at 300 K, how small can a grain be?
Show the solution
- The stability condition. Thermal fluctuations flip a grain over its anisotropy barrier KV at a rate of about per second, so ten years of stability needs KV of roughly 60kT.
- Smallest volume. a cube 7.9 nm on a side.
- Smaller grains. Smaller grains are superparamagnetic: their moments wander thermally.
- Higher anisotropy. Higher K holds smaller grains but needs stronger write fields, which is why heat-assisted recording warms each bit briefly while writing it.
Answer a grain can be no smaller than about 497 nm³, a cube 7.9 nm on a side.
Check
A ferromagnet has 9.1 × 10²⁸ magnetic atoms per m³, each contributing 2.22 Bohr magnetons. What's its saturation flux density ?
Write units the way you normally would: 1.5 T, 1500 mT and 0.0015 kT are the same answer.
Check
A core (saturation 0.3 T, coercivity 5 A/m, volume 20 cm³) is driven around its full square-ish loop at 100000 Hz. How much power does hysteresis waste?
Write units the way you normally would: 1.5 W, 1500 mW and 0.0015 kW are the same answer.
Check
A 120 V, 50 Hz winding has 500 turns on a 20 cm² core. What's the peak flux density?
Write units the way you normally would: 1.5 T, 1500 mT and 0.0015 kT are the same answer.
Check
A permanent magnet has remanence 1.2 T. What's the largest energy product it could have?
Write units the way you normally would: 1.5 kJ/m^3, 1500 J/m^3 and 0.0015 MJ/m^3 are the same answer.
Check
In the model loop with saturation 1.6 T, coercivity 10 A/m and softness 25 A/m, what's the remanence?
Write units the way you normally would: 1.5 T, 1500 mT and 0.0015 kT are the same answer.
Check
Why are ferrites, rather than iron, used for cores at hundreds of kilohertz?
Check
A recording grain has anisotropy 0.5 MJ/m³ at 300 K and must keep KV ≥ 60kT.
(a)
What's the smallest stable volume?
(b)
How big a cube is that?
Write units the way you normally would: 1.5 nm, 1500 pm and 0.0015 µm are the same answer.
Check
A ferromagnet has n magnetic atoms per m³, each with p Bohr magnetons.
Step 1
What's its saturation magnetization, in A/m?
Type it the way you would write it, like 3sin(2πft) or 3*sin(2*pi*f*t). Angles can be in radians or carry a degree sign, like 45°.
Step 2
What's its saturation flux density , in tesla?
Explain why
What makes a ferromagnet's spins line up spontaneously when a paramagnet's don't?
In a paramagnet the moments are independent, and only an external field aligns them, against thermal disorder. In a ferromagnet, neighboring electrons interact through exchange: because of the Pauli principle, the electrostatic repulsion between two electrons depends on whether their spins are parallel or antiparallel, and in iron, cobalt and nickel parallel spins have the lower energy. This coupling is far stronger than the magnetic interaction between the moments themselves, equivalent to an internal field of hundreds of tesla. Below the Curie temperature it wins over thermal agitation and all the spins in a domain align, even with no field applied; above it, thermal energy breaks the order and the material becomes paramagnetic.