D6 · Lesson 6 · Fabrication
How a transistor is built up layer by layer on a wafer, oxidation, lithography and its resolution limit, etching, deposition and polishing, ion implantation with its dose, peak concentration and junction depth, annealing, and the metal wiring stacked on top
A modern chip is built in about a thousand process steps over two or three months. The same few operations repeat dozens of times: coat the wafer, print a pattern in light, etch or implant where the pattern allows, strip the resist, clean, inspect. Each pass adds one layer, defined to a few nanometers across a wafer 300 mm wide. Doping, the step that turns silicon into transistors, is done by firing ions into the wafer like microscopic bullets, and their depth is controlled by their energy.
- The concentration profile of boron implanted into n-type silicon: a Gaussian of dose Q (atoms per cm²) centered at the projected range with straggle , over a background doping .
- The junction is where the implanted boron falls to the background: shallow implants need low energy (small ) and light doses.
- The readouts give the peak concentration and the junction depth.
Predict
A dose of boron atoms per cm² is implanted with a straggle of 20 nm. What's the peak concentration?
The dose is spread over a Gaussian of width = 2.507 × 2 × 10⁻⁶ cm = 5.0 × 10⁻⁶ cm, so the peak is 10¹⁵/5.0 × 10⁻⁶ = 2.0 × 10²⁰ cm⁻³, enough for a low-resistance source or drain. With = 50 nm on a 10¹⁷ background, the junction is 128 nm deep.
Name it
The process loop
- Oxidation or deposition adds a film: thermal SiO₂, silicon nitride, polysilicon, metals, high-κ dielectrics deposited an atomic layer at a time.
- Lithography coats the wafer with photoresist and exposes it through a mask. The smallest printable half-pitch is about
with wavelength λ, numerical aperture NA and process factor . 193 nm immersion scanners (NA 1.35) reach about 40 nm in one exposure; extreme-ultraviolet scanners at 13.5 nm reach about 16 nm at NA 0.33 and under 10 nm at NA 0.55. Smaller features use multiple patterning.
- Etching removes material where the resist is open; plasma etching cuts straight down.
- Implantation fires dopant ions into the open areas, then an anneal repairs the crystal damage and activates the dopants.
- Chemical-mechanical polishing flattens the surface for the next layer.
Ion implantation
A dose Q (ions per cm²) lands in a roughly Gaussian profile:
The junction lies where N(x) equals the background :
The dose is counted electrically: a beam current I for time t over area A delivers .
Front end and back end
The front end builds the transistors in the silicon. The back end stacks up to fifteen or more levels of copper wiring in insulating layers above them, connected by vias, which is where most of the steps and masks now go.
Worked example
How long does a 1 mA beam take to implant cm⁻² over a 300 mm wafer?
Show the solution
- Wafer area.
- Charge needed.
- Time at 1 mA.
Answer the implant takes 113 s.
Worked example
What half-pitch can a 193 nm immersion scanner print with = 0.28, and an EUV scanner with = 0.4?
Show the solution
- 193 nm immersion. The half-pitch is :
- EUV.
- High-NA EUV.
Answer 40 nm with 193 nm immersion, 16.4 nm with EUV, and 9.8 nm with high-NA EUV.
Worked example
Boron diffuses with D ≈ 1.5 × 10⁻¹⁴ cm²/s at 1000 °C. How far does it spread in a one-hour anneal?
Show the solution
- Diffusion length. and a profile's edge moves by a few of those.
- For modern transistors. With 20 nm features that's far too much, so modern processes anneal in milliseconds (spike and flash anneals).
Answer the diffusion length is 73 nm, and the profile's edge moves a few times that.
Check
A dose of cm⁻² is implanted with a straggle of 10 nm. What's the peak concentration?
Check
A cm⁻² implant has = 30 nm and = 30 nm, into a background of cm⁻³. How deep is the junction?
Write units the way you normally would: 1.5 nm, 1500 pm and 0.0015 µm are the same answer.
Check
A scanner has wavelength 13.5 nm and numerical aperture 1.35, and the process achieves = 0.3. What half-pitch can it print?
Write units the way you normally would: 1.5 nm, 1500 pm and 0.0015 µm are the same answer.
Check
How long does a 0.1 mA beam take to implant a dose of cm⁻² over a 300 mm wafer?
Write units the way you normally would: 1.5 s and 1500 ms are the same answer.
Check
An implant of cm⁻², Q = 5, covers a 300 mm wafer with a 0.5 mA beam.
(a)
How much charge must arrive?
Write units the way you normally would: 1.5 C, 1500 mC and 0.0015 kC are the same answer.
(b)
How long does it take?
Check
A dopant diffuses with cm²/s for 10 s.
(a)
What is its diffusion length?
Write units the way you normally would: 1.5 nm, 1500 pm and 0.0015 µm are the same answer.
(b)
What would it be after four times as long?
Explain why
Why does lithography, more than any other step, set how small transistors can be?
Every feature on a chip is defined by a pattern printed in photoresist, and the smallest pattern an optical system can print is limited by diffraction to roughly the wavelength divided by the lens's numerical aperture, times a process factor that clever masks and resists can push down only to about a quarter. Etching, deposition and implantation can follow whatever pattern they're given with nanometer precision, but they can't make a feature finer than the one printed. So each new generation needed a shorter wavelength, a larger aperture or tricks such as immersion in water and multiple patterning, and the move to 13.5 nanometer extreme-ultraviolet light was the largest and costliest change in the industry's history.
Practice
Keep practicing
8 kinds of problem on this topic, dealt one at a time with new numbers every time, for as long as you like.