title: Fabrication
heading: How a transistor is built up layer by layer on a wafer, oxidation, lithography and its resolution limit, etching, deposition and polishing, ion implantation with its dose, peak concentration and junction depth, annealing, and the metal wiring stacked on top
eyebrow: D6 · Lesson 6 · Fabrication
xp: 40
---

::: hook
A modern chip is built in about a thousand process steps over two or three months. The same few operations repeat dozens of times: coat the wafer, print a pattern in light, etch or implant where the pattern allows, strip the resist, clean, inspect. Each pass adds one layer, defined to a few nanometers across a wafer 300 mm wide. Doping, the step that turns silicon into transistors, is done by firing ions into the wafer like microscopic bullets, and their depth is controlled by their energy.
:::

::: play
- The concentration profile of boron implanted into n-type silicon: a Gaussian of dose Q (atoms per cm²) centered at the projected range $R_p$ with straggle $\Delta R_p$, over a background doping $N_B$.
- The **junction** is where the implanted boron falls to the background: shallow implants need low energy (small $R_p$) and light doses.
- The readouts give the peak concentration and the junction depth.
:::

```sim plot
view: graph
x: x = 0..400
y: N = 1e14..1e21 log
slider: Q = 12..16 step 0.1 = 15
slider: R = 10..150 step 5 = 50
slider: s = 5..60 step 1 = 20
slider: B = 15..18 step 0.1 = 17
plot: 10^Q/(sqrt(2*pi)*s*1e-7)*exp(-(x - R)^2/(2*s^2)) | samples: 500 | label: implanted boron, cm⁻³ (x in nm)
plot: 10^B + 0*x | dashed | color: ch3 | label: background doping
readout: peak concentration, cm⁻³ = 10^Q/(sqrt(2*pi)*s*1e-7) | digits: 3
readout: junction depth, nm = R + s*sqrt(2*ln(10^Q/(sqrt(2*pi)*s*1e-7)/10^B)) | digits: 4
```

::: predict
## A dose of $10^{15}$ boron atoms per cm² is implanted with a straggle of 20 nm. What's the peak concentration?

- [ ] $10^{15}$ cm⁻³
- [ ] $10^{17}$ cm⁻³
- [x] About $2 \times 10^{20}$ cm⁻³
- [ ] About $10^{23}$ cm⁻³

::: reveal
The dose is spread over a Gaussian of width $\sqrt{2\pi}\Delta R_p$ = 2.507 × 2 × 10⁻⁶ cm = 5.0 × 10⁻⁶ cm, so the peak is 10¹⁵/5.0 × 10⁻⁶ = 2.0 × 10²⁰ cm⁻³, enough for a low-resistance source or drain. With $R_p$ = 50 nm on a 10¹⁷ background, the junction is 128 nm deep.
:::
:::

::: nameit
## The process loop

1. **Oxidation or deposition** adds a film: thermal SiO₂, silicon nitride, polysilicon, metals, high-κ dielectrics deposited an atomic layer at a time.
2. **Lithography** coats the wafer with photoresist and exposes it through a mask. The smallest printable half-pitch is about
$$R = k_1\frac{\lambda}{NA}$$
with wavelength λ, numerical aperture NA and process factor $k_1 \ge 0.25$. 193 nm immersion scanners (NA 1.35) reach about 40 nm in one exposure; extreme-ultraviolet scanners at 13.5 nm reach about 16 nm at NA 0.33 and under 10 nm at NA 0.55. Smaller features use multiple patterning.
3. **Etching** removes material where the resist is open; plasma etching cuts straight down.
4. **Implantation** fires dopant ions into the open areas, then an **anneal** repairs the crystal damage and activates the dopants.
5. **Chemical-mechanical polishing** flattens the surface for the next layer.

## Ion implantation

A dose Q (ions per cm²) lands in a roughly Gaussian profile:

$$N(x) = \frac{Q}{\sqrt{2\pi}\Delta R_p}e^{-(x - R_p)^2/2\Delta R_p^2}$$

The junction lies where N(x) equals the background $N_B$:

$$x_j = R_p + \Delta R_p\sqrt{2\ln\frac{N_\text{peak}}{N_B}}$$

The dose is counted electrically: a beam current I for time t over area A delivers $Q = It/(qA)$.

## Front end and back end

The **front end** builds the transistors in the silicon. The **back end** stacks up to fifteen or more levels of copper wiring in insulating layers above them, connected by vias, which is where most of the steps and masks now go.
:::

::: example
## How long does a 1 mA beam take to implant $10^{15}$ cm⁻² over a 300 mm wafer?

::: solution
1. **Wafer area.**
   $$\pi \times 15^2 = 706.9\ \text{cm}^2$$
2. **Charge needed.**
   $$\begin{aligned} QqA &= 10^{15} \times 1.602 \times 10^{-19} \\ &\quad \times 706.9\ \text{C} \\ &= 0.113\ \text{C} \end{aligned}$$
3. **Time at 1 mA.**
   $$\frac{0.113\ \text{C}}{1\ \text{mA}} = 113\ \text{s}$$

**Answer:** the implant takes 113 s.
:::
:::

::: example
## What half-pitch can a 193 nm immersion scanner print with $k_1$ = 0.28, and an EUV scanner with $k_1$ = 0.4?

::: solution
1. **193 nm immersion.** The half-pitch is $k_1\lambda/\text{NA}$:
   $$0.28 \times \frac{193\ \text{nm}}{1.35} = 40\ \text{nm}$$
2. **EUV.**
   $$0.4 \times \frac{13.5\ \text{nm}}{0.33} = 16.4\ \text{nm}$$
3. **High-NA EUV.**
   $$0.4 \times \frac{13.5\ \text{nm}}{0.55} = 9.8\ \text{nm}$$

**Answer:** 40 nm with 193 nm immersion, 16.4 nm with EUV, and 9.8 nm with high-NA EUV.
:::
:::

::: example
## Boron diffuses with D ≈ 1.5 × 10⁻¹⁴ cm²/s at 1000 °C. How far does it spread in a one-hour anneal?

::: solution
1. **Diffusion length.**
   $$\begin{aligned} \sqrt{Dt} &= \sqrt{1.5 \times 10^{-14} \times 3600}\ \text{cm} \\ &= 7.3 \times 10^{-6}\ \text{cm} \\ &= 73\ \text{nm} \end{aligned}$$
   and a profile's edge moves by a few of those.
2. **For modern transistors.** With 20 nm features that's far too much, so modern processes anneal in milliseconds (spike and flash anneals).

**Answer:** the diffusion length is 73 nm, and the profile's edge moves a few times that.
:::
:::

::: check
given: e = 13 | 14 | 15; s = 10 | 20 | 40
answer: 10^e/(sqrt(2*pi)*s*1e-7)
unit: cm⁻³
tolerance: 0.5%

## A dose of $10^{\given{e}}$ cm⁻² is implanted with a straggle of {s} nm. What's the peak concentration?

::: right
Right. $Q/(\sqrt{2\pi}\Delta R_p)$ = {answer} cm⁻³.
:::

::: misses
- [10^e/(s*1e-7)] Divide by $\sqrt{2\pi}\Delta R_p$, the Gaussian's effective width.
- [any] Not yet. Spread the dose over the profile.
:::
:::

::: check
given: e = 14 | 15; R = 30 | 80; s = 15 | 30; b = 16 | 17
answer: R + s*sqrt(2*ln(10^e/(sqrt(2*pi)*s*1e-7)/10^b))
unit: nm
tolerance: 0.5%

## A $10^{\given{e}}$ cm⁻² implant has $R_p$ = {R} nm and $\Delta R_p$ = {s} nm, into a background of $10^{\given{b}}$ cm⁻³. How deep is the junction?

::: right
Right. $R_p + \Delta R_p\sqrt{2\ln(N_\text{peak}/N_B)}$ = {answer} nm.
:::

::: misses
- [R] That's the peak; the junction lies deeper, where the tail meets the background.
- [any] Not yet. Find the peak, then solve N(x) = $N_B$.
:::
:::

::: check
given: k = 0.25 | 0.3 | 0.4; w = 13.5 | 193; n = 0.33 | 0.55 | 1.35
answer: k*w/n
unit: nm
tolerance: 0.5%

## A scanner has wavelength {w} nm and numerical aperture {n}, and the process achieves $k_1$ = {k}. What half-pitch can it print?

::: right
Right. $k_1\lambda/NA$ = {answer} nm.
:::

::: misses
- [w/n] Multiply by $k_1$.
- [any] Not yet. The Rayleigh resolution.
:::
:::

::: check
given: e = 13 | 14 | 15; I = 0.1 | 1 | 10; d = 200 | 300
answer: 10^e*1.602e-19*pi*(d/20)^2/(I*1e-3)
unit: s
tolerance: 0.5%

## How long does a {I} mA beam take to implant a dose of $10^{\given{e}}$ cm⁻² over a {d} mm wafer?

::: right
Right. $QqA/I$ = {answer} s.
:::

::: misses
- [any] Not yet. Total charge needed, over the beam current.
:::
:::

::: check
kind: parts
given: Q = 1 | 5 | 10; I = 0.5 | 1 | 10; d = 200 | 300

## An implant of $Q \times 10^{14}$ cm⁻², Q = {Q}, covers a {d} mm wafer with an {I} mA beam.

::: part
answer: Q*1e14*1.602e-19*pi*(d/20)^2
unit: C
tolerance: 0.5%

### How much charge must arrive?

::: misses
- [any] Dose × q × area.
:::
:::

::: part
answer: Q*1e14*1.602e-19*pi*(d/20)^2/(I/1000)
unit: s
tolerance: 0.5%

### How long does it take?

::: misses
- [any] Charge ÷ current.
:::
:::
:::

::: check
kind: parts
given: D = 1 | 5 | 20; t = 10 | 60 | 3600

## A dopant diffuses with $D = \given{D} \times 10^{-15}$ cm²/s for {t} s.

::: part
answer: sqrt(D*1e-15*t)*1e7
unit: nm
tolerance: 0.5%

### What is its diffusion length?

::: misses
- [any] $\sqrt{Dt}$.
:::
:::

::: part
answer: sqrt(D*1e-15*4*t)*1e7
unit: nm
tolerance: 0.5%

### What would it be after four times as long?

::: misses
- [any] Twice as far: it grows as $\sqrt t$.
:::
:::
:::

::: explain
## Why does lithography, more than any other step, set how small transistors can be?

::: model
Every feature on a chip is defined by a pattern printed in photoresist, and the smallest pattern an optical system can print is limited by diffraction to roughly the wavelength divided by the lens's numerical aperture, times a process factor that clever masks and resists can push down only to about a quarter. Etching, deposition and implantation can follow whatever pattern they're given with nanometer precision, but they can't make a feature finer than the one printed. So each new generation needed a shorter wavelength, a larger aperture or tricks such as immersion in water and multiple patterning, and the move to 13.5 nanometer extreme-ultraviolet light was the largest and costliest change in the industry's history.
:::
:::

::: practice

::: check
given: e = 11 | 12 | 13 | 14 | 15 | 16; s = 5 | 100
answer: 10^e/(sqrt(2*pi)*s*1e-7)
unit: cm⁻³
tolerance: 0.5%

## Peak from $10^{\given{e}}$ cm⁻², straggle {s} nm?

::: misses
- [any] $Q/(\sqrt{2\pi}\Delta R_p)$.
:::
:::

::: check
given: k = 0.25 | 0.6; w = 13.5 | 193 | 248 | 365; n = 0.3 | 1.35
answer: k*w/n
unit: nm
tolerance: 0.5%

## Half-pitch: $k_1$ = {k}, λ = {w} nm, NA = {n}?

::: misses
- [any] $k_1\lambda/NA$.
:::
:::
:::