D6 · Lesson 9 · Capstone
Putting the steps of a CMOS process in their working order, matching each tool to its job, and then following one step closely in code, an implanted and annealed source and drain, to see how the anneal moves the junction while leaving the sheet resistance almost untouched
A process engineer's job is to put hundreds of steps in an order where each one works: you can't etch a gate before you've deposited it, implant a source before the gate exists to mask it, or heat the wafer to 1000 °C after the copper is in. This capstone asks you to assemble the core of a CMOS flow, then zoom in on one step that every transistor depends on, the source and drain implant and its anneal, and compute in code what it does to the junction and the resistance.
- An n⁺ source/drain implant ( cm⁻² at a projected range of 80 nm with 20 nm straggle) in a cm⁻³ p-type well, and the same profile after an anneal of t seconds at diffusivity D (in units of cm²/s).
- The anneal spreads the Gaussian, lowering its peak and pushing the junction deeper, while the dose under the curve stays the same.
- Long, hot anneals push junctions too deep for short transistors: modern processes use millisecond and spike anneals.
Predict
A 60 s anneal at cm²/s widens the 20 nm straggle. To what?
Diffusion adds 2Dt to the Gaussian's variance: 2 × 1.4 × 10⁻¹⁴ × 60 = 1.68 × 10⁻¹² cm², or 168 nm², so the straggle becomes √(400 + 168) = 23.8 nm. The junction moves from 165.8 nm to 181.3 nm deep, while the sheet resistance hardly changes, as the Python step below shows.
Check
Put these steps of a simplified CMOS front end in order, first to last.
- Implant the sources and drains, using the gates as masks
- Pattern and etch the isolation trenches
- Deposit insulator, etch contact holes and fill them with tungsten
- Pattern and etch the gates
- Implant the n-wells and p-wells
- Build the copper wiring levels
- Fill the trenches with oxide and polish the wafer flat
- Anneal to repair the crystal and activate the dopants
- Grow a thin pad oxide and deposit silicon nitride
- Grow the gate dielectric and deposit the gate material
Check
Match each tool to its job.
- APlaces dopants at a chosen depth
- BGrows a film one atomic layer at a time
- CDefines where the next step acts
- DFlattens the surface
- ERemoves material straight down through openings
- FRepairs damage and activates dopants
Name it
Why this order
- Isolation first: shallow trenches filled with oxide separate neighboring transistors and must exist before anything is built between them.
- Wells next: deep, light implants set each transistor's body type and threshold.
- Self-aligned gates: the gate is patterned before the source and drain, so it masks the channel during their implant, aligning every source and drain to its gate without a second lithography step. (Advanced processes replace the polysilicon later with a metal gate.)
- Heat before metal: activation anneals reach 1000 °C or more, so they precede silicide, tungsten contacts and copper wiring, which tolerate only about 400 °C.
The source/drain step
The implant is a Gaussian of dose Q at depth with straggle (lesson 6). An anneal with diffusivity D for time t widens it to
with the dose unchanged, which lowers the peak and deepens the junction. The sheet resistance, in ohms per square, is
For a dose of cm⁻² and mobility near 95 cm²/V·s at cm⁻³, about 13 Ω/□. Since the dose is fixed and mobility hardly changes at such heavy doping, the anneal barely moves .
Worked example
What's the rough sheet resistance of the cm⁻² source/drain, and the junction depth before the anneal?
Show the solution
- Rough sheet resistance. With q = 1.602 × 10⁻¹⁹ C, μ = 95 cm²/V·s and Q = 5 × 10¹⁵ cm⁻²: (the careful integral gives 13.44).
- Peak concentration.
- Junction depth. The profile falls to the background times below the peak:
Answer about 13.1 Ω/□ (13.44 by the careful integral), and a junction depth of 165.8 nm before the anneal.
Worked example
An implant of cm⁻² has a 20 nm straggle. What is its peak concentration?
Show the solution
- Peak of a Gaussian. A Gaussian of dose Q and straggle ΔR peaks at
- Five times the dose. Five times the dose gives five times the peak, the of the source and drain.
Answer the peak is cm⁻³.
Check
Model the implant and the anneal, find the junction, and integrate the sheet resistance.
Python 3.14 with numpy and matplotlib, running in your browser. Tab indents; press Esc and then Tab to move on.
Check
An implant with 20 nm of straggle is annealed for 600 s at = 0.5 × cm²/s. What's its new straggle?
Write units the way you normally would: 1.5 nm, 1500 pm and 0.0015 µm are the same answer.
Check
About what sheet resistance does an n-type layer with a dose of cm⁻² and an average mobility of 90 cm²/V·s have, in ohms per square?
Write units the way you normally would: 1.5 Ω, 1500 mΩ and 0.0015 kΩ are the same answer.
Check
An implant of cm⁻², Q = 5, has a straggle of 10 nm.
(a)
What is its peak concentration?
(b)
Roughly what sheet resistance does it give, with a mobility of 95 cm²/V·s?
Write units the way you normally would: 1.5 Ω, 1500 mΩ and 0.0015 kΩ are the same answer.
Check
An implant peaks at depth 50 nm with straggle 15 nm, into a background 100000 times below its peak.
(a)
At what depth does it fall to the background (the junction)?
Write units the way you normally would: 1.5 nm, 1500 pm and 0.0015 µm are the same answer.
(b)
How far below the peak is that?
Explain why
Why must the source and drain be implanted after the gate is patterned?
The gate sits over the channel, and the source and drain must begin exactly at its edges: any gap would leave an ungated, high-resistance stretch, and any overlap adds capacitance between the gate and the source or drain. Implanting after the gate is patterned lets the gate itself act as the mask, since the ions can't get through it into the channel underneath, so each source and drain lines up with its own gate automatically, with no second alignment that could be a few nanometers off. This self-alignment is one of the key ideas that made dense CMOS manufacturable, and it fixes the order of the gate and the source and drain steps.
Practice
Keep practicing
6 kinds of problem on this topic, dealt one at a time with new numbers every time, for as long as you like.